Evaluating the Effects of Sandblasting on Micro-Shear Bond Strength and Flexural Strength of Zirconia
(ندگان)پدیدآور
Majidinia, SBagheri, HMaghsoudlou Nejad, MShekofteh, KParhizkar, Tنوع مدرک
TextExperimental
زبان مدرک
Englishچکیده
Background and Objective: Various techniques have been introduced to improve bond strength of zirconia which may negatively affect flexural strength. This study aims to evaluate the effects of different sandblasting parameters on micro-shear bond strength (MSBS, Mpa) and biaxial flexural strength (BFS, Mpa) of Zirconia.
Methods: In this in vitro study, zirconia blocks were cut into 180 discs for MSBS and BFS tests (90 specimens in each group). For each test, they were divided into one control group and 8 experimental groups according to the type of sandblasting regimen (pressures of 4 or 6 bar, duration of 14 or 21 seconds, and alumina powder sizes of 50 or 110 μm, n=10). A universal testing machine was used to determine MSBS and BFS. X-ray diffraction (XRD) analysis was then performed.
Findings: According to the results, groups with 110 μm particles (4 bar- 14 s, 6 bar- 14 s, 4 bar- 21 s and 6 bar- 21 s with MSBS values of 34.43±5.99, 35.21±6.39, 27.17±3.95 and 28.66±3.92 Mpa, respectively) had significantly higher MSBS values compared to the control group (p
کلید واژگان
Flexural StrengthX-Ray Diffraction
Yttria-Stabilized Tetragonal Zirconia
Air Abrasion.
شماره نشریه
1تاریخ نشر
2022-03-011400-12-10
ناشر
دانشگاه علوم پزشکی بابلسازمان پدید آورنده
1.Dental Materials Research Center, Mashhad University of Medical Sciences, Mashhad, I.R.Iran.1.Dental Materials Research Center, Mashhad University of Medical Sciences, Mashhad, I.R.Iran.
2.Department of Restorative Dentistry, School of Dentistry, Mashhad University of Medical Sciences, Mashhad, I.R.Iran.
3.Department of Dental Biomaterials, School of Dentistry, Tehran University of Medical Sciences, Tehran, I.R.Iran.
1.Dental Materials Research Center, Mashhad University of Medical Sciences, Mashhad, I.R.Iran.
شاپا
1561-41072251-7170